Unvulcanized rubber compounds
In the most general form of crude rubber mixture contains the following components: a mixture of rubber or rubbers curing system, fillers, plasticizers (softeners), stabilizers, antioxidants. Depending on the chemical composition of a type of rubber becomes possible to manufacture a great variety of technical rubber products, ranging from ordinary seals, and high quality finishing of car tires. With the tire vulcanizing crude converted into a finished product. When exposed to high temperatures in the raw chemical reactions occurring at the molecular level. This product has high elasticity and flexibility, it is able to perform complex plastic deformation, thereby becoming indispensable, extremely practical and versatile material that has found its application in industry and in everyday life.
Crude rubber - the basis for the production of various kinds of rubber products. Our company puts its own products a lot of testing before products get to the customer. Rubber compounds have good chemical resistance, resistance to wear and impact of external mechanical damage. These qualities give the product excellent performance characteristics. Different mixtures are used in various environments. Some of them are used for making sealing or other kinds of products which can be used in air, the aqueous media, dilute solutions of acids, alkalis. Exceptions are acetic acid and nitric acid. Others - for a variety of articles of manufacture that are used in contact with the fuel or oil.
Depending on the purpose and conditions of the products rubber compounds are classified:
hardness:
• soft,
• solid
• increased hardness
the method of production:
• rolled
• calendered
Trademarks uncured rubber compounds on TU 6 00152135.040-96
Group of rubber |
Rubber stamps |
Rubber type |
Shore Temp. |
Temperature interval |
|
|||
|
||||||||
Soft |
||||||||
I -м |
7-ВЛ-44 |
СКМС-30АРКМ-15 |
40-55 |
-30 tо +70 |
Air, water, weak acids and alkali solutions to a concentration of 20% by volume (except for acetic acid and nitric) |
|||
I -м |
2658 |
СКМС-30АРКМ-15+ регенерат |
45-60 |
-35 tо +70 |
||||
I -м |
7-6721 |
СКМС-30АРКМ-15+ СКД |
40-55 |
-30 tо +70 |
||||
I -м |
ИРП-1346 |
СКИ-3+СКД |
40 -50 |
-50 tо+70 |
||||
I -м |
7-2959 |
НК |
45-60 |
-45 tо +70 |
||||
I -м |
ИРП-1365 |
СКИ-3 |
40-55 |
-30 tо +70 |
||||
Half-hard |
||||||||
I -с |
7-122 |
СКМС-30АРКМ-15+ СКД, регенерат |
65-75 |
-40 to +80 |
Air, water, weak acids and alkali solutions to a concentration of 20% by volume (except for acetic acid and nitric) |
|||
I -с |
51-3060 |
СКИ-3 |
50-70 |
-40 tо +80 |
||||
I -с |
6620 |
СКИ-3+СКД |
50-60 |
-45 tо +80 |
||||
I -с |
199 |
СКМС-30АРКМ-15 |
60-70 |
-35 tо +80 |
||||
I -с |
6550 |
СКМС-30АРКМ-15+СКД |
50-65 |
-45 tо +80 |
||||
I -с |
6722 |
СКМС-30АРКМ-15+СКД |
55-70 |
-45 tо +80 |
||||
I -с |
6429 |
СКМС-30АРКМ-15 |
50-65 |
-35 tо +80 |
||||
I -с |
Кр-407 |
СКМС-30АРКМ-15 |
50-65 |
-35 tо +80 |
||||
I -с |
Су-360 |
СКМС-30АРКМ-15 |
50-65 |
-30 tо +70 |
||||
I -с |
6190 |
СКМС-30АРКМ-15 |
60-75 |
-35 tо +80 |
||||
I -с |
6322 |
СКМС-30АРКМ-15 |
50-65 |
-45 tо +80 |
||||
I -с |
2675 |
СКМС-30АРКМ-15 |
50-65 |
-50 tо +80 |
||||
Increased hardness |
||||||||
I -п |
ИРП -1348 |
СКИ-3+СКД |
65-80 |
-55 tо +125 |
Air, water, weak acids and alkali solutions to a concentration of 20% by volume (except for acetic acid and nitric) |
|||
I -п |
7-2462 |
НК |
60-75 |
-45 tо +80 |
||||
I -п |
7-120 |
СКИ-3 |
65-75 |
-45 tо +80 |
||||
|
|
|
|
|
|
|||
I I . Rubber compoundsfor theproduction of sealingand otherproducts operatingin coldclimates.
|
||||||||
Soft |
||||||||
II -м |
ИРП-1346 |
СКИ-3+СКД |
40 -50 |
-50 tо+70 |
The air in cold climates |
|||
II-м |
6620 |
СКИ-3+СКД |
40-50 |
-50 tо+70 |
||||
Half-hard |
||||||||
II-с |
ИРП-1347 |
СКИ-3+СКД |
47-57 |
-50 tо + 70 |
The air in cold climates |
|||
II -с |
14к-10 |
СКМС-10 |
50-65 |
-50 tо +70 |
||||
|
|
|
|
|
|
|||
Increased hardness |
||||||||
II -п |
ИРП-1348 |
СКИ-3+СКД |
65-80 |
-50 tо +70 |
The air in cold climates |
|||
II -п |
ИРП-1231 |
СКИ-3+СКД, СКМС-30АРКМ-15 |
65-80 |
-50 tо +70 |
||||
|
|
|
|
|
|
|||
III . Rubber compoundsfor theproduction of sealingand otherproducts operatingin contactwith oils andfuels |
||||||||
1. limited petrol and oil resistant |
||||||||
Soft |
||||||||
III-1м |
4161 |
БНКС-28(СКН-26) |
40-55 |
-25 tо +100 |
In contact with oils and fuels |
|||
III-1м |
9-9073 |
СКН-26 |
40-55 |
-25 tо +100 |
||||
|
|
|
|
|
|
|||
Half-hard. |
||||||||
III -1с |
8470 |
БНКС-18+ БНКС-28 |
50-65 |
-30 tо +100 |
В In contact with oils and fuels |
|||
III -1с |
НО-68 |
БНКС-18+хлоропреновый |
50-70 |
-50 tо +100 |
||||
III -1с |
52-509 |
БНКС-18 |
50-70 |
-35 tо +100 |
||||
III -1с |
7-ИРП-1352 |
БНКС-18 |
50-70 |
-30 tо +100 |
||||
III -1с |
9003 |
БНКС-18 |
50-70 |
-30 tо +100 |
||||
|
|
|
|
|
|
|||
Increased hardness |
||||||||
III -1п |
7-В-14 |
БНКС-18АМН (СКН-18) |
70-80 |
-45 tо +100 |
In contact with oils and fuels |
|||
III -1п |
4326 |
СКН-18 |
65-80 |
-45 tо +100 |
||||
III -1п |
7-7130 |
СКН-18 |
60-85 |
-45 tо +100 |
||||
III -1п |
6659 |
БНКС-18 |
60-85 |
-45 tо +100 |
||||
III -1п |
2542 |
хлоропреновый |
60-85 |
-40 tо +100 |
||||
III -1п |
3465 |
хлоропреновый |
60-85 |
-35 tо +100 |
||||
|
|
|
|
|
|
|||
2. Half petrol and oil resistant |
||||||||
Soft |
||||||||
III -2м |
3824 |
СКН-26 |
35-55 |
-30 tо +100 |
In contact with oils and fuels |
|||
III -2м |
8470 |
БНКС-18+ БНКС-40 |
35-55 |
-30 tо +100 |
||||
III -2м |
4161 |
СКН-26 |
40-55 |
-30 tо +100 |
||||
III -2м |
9024 |
СКН-26+ БНКС |
35-55 |
-30 to +100 |
||||
|
|
|
|
|
|
|||
Half-hard |
||||||||
III -2с |
9831 |
СКН-18+ СКН-26 |
55-70 |
-30 tо +100 |
In contact with oils and fuels |
|||
III -2с |
51-3050 |
СКН-26МП |
50-70 |
-30 tо +100 |
||||
III -2с |
ИРП-1293 |
СКН-26 |
50-70 |
-30 tо +100 |
||||
|
|
|
|
|
||||
Increased hardness |
||||||||
III -2п |
51-3029 |
СКН-18+СКН-26С |
60-90 |
-30 tо +100 |
In contact with oils and fuels |
|||
III -2п |
7-3825 |
БНКС-18+ БНКС-40 |
60-90 |
-30 tо +100 |
||||
III -2п |
ИРП-1078 |
СКН-18+СКН-26С |
75-85 |
-30 tо +100 |
||||
III -2п |
ИРП-1068 |
СКН-26 |
75-90 |
-30 tо +100 |
||||
III -2п |
7-3465 |
хлоропреновый |
60-90 |
-35 tо +100 |
||||
III -2п |
7-8075 |
СКН-18+СКН-26С |
60-90 |
-35 tо +100 |
||||
|
|
|
|
|
|
|||
3. Increased petrol and oil resistant |
||||||||
Soft |
||||||||
III -3м |
7-3834 |
СКН-40 + БНКС |
40-55 |
-20 tо +100 |
In contact with oils and fuels |
|||
|
|
|
|
|
||||
Half-hard |
||||||||
III -3с |
7-3826 |
СКН-40 |
60-75 |
-20 tо +100 |
In contact with oils and fuels |
|||
III -3с |
7-3825 |
СКН-40 + БНКС-18 |
50-70 |
-20 tо +100 |
||||
III -3с |
4004 |
СКН-40 |
50-70 |
-15 tо +125 |
||||
|
|
|
|
|
|
|||
|
|
|
|
|
|
|||
Increased hardness |
||||||||
III -3п |
ИРП-1293 |
СКН-40 |
65-80 |
-30 tо +100 |
In contact with oils and fuels |
|||
III -3п |
3825 |
БНКС-18+ БНКС-40 |
65-80 |
-30 tо +100 |
||||
III-3п |
Кр-360 |
СКН-26 |
65-90 |
-30 tо +100 |
||||
III-3п |
Кз-694 |
СКН-40 |
75-90 |
-20 tо +100 |
||||
III-3п |
7223 |
БНКС |
65-95 |
-15 tо +125 |
||||
|
|
|
|
|
|
|||
IV. Rubbercomposition forproduction of varioussealsand other products |
||||||||
Soft |
||||||||
IV-м |
ИРП-1352 |
СКН-18 |
35-65 |
-50 tо +100 |
In contact with oils and fuel in cold climates |
|||
Half-hard |
||||||||
IV-с |
98-1 |
СКН-18С |
50-65 |
-50 tо +100 |
In contact with oils and fuel in cold climates |
|||
IV-с |
Г-34 |
СКН-18С |
55-70 |
-50 до +100 |
||||
Increased hardness |
||||||||
IV- п |
51-3028 |
СКН-18С |
75-90 |
-50 tо +100 |
In contact with oils and fuel in cold climates |
|||
IV- п |
В-14-1 |
СКН-18С |
75-85 |
-50 tо +100 |
||||
|
|
|
|
|
|
|||
V. Rubbercomposition forproduction of varioussealsand other products |
||||||||
Soft |
||||||||
V-м |
57-7018 |
СКЭПТ-40,50 |
45-65 |
-50 tо +125 |
In an environment of air, ozone, light, hot water |
|||
Half-hard |
||||||||
V-с |
66-415 |
СКЭПТ-30,40 |
60-75 |
-50 tо +80 |
In an environment of air, ozone, light, hot water |
|||
V-с |
51-1510 |
СКЭПТ-40,50 |
60-75 |
-50 tо +80 |
||||
|
|
|
|
|
|
|||
Increased hardness |
||||||||
V-п |
51-1481 |
СКЭПТ-40,50 |
75-90 |
-50 tо +125 |
In an environment of air, ozone, light, hot water |
|||
|
|
|
|
|
||||
VI. Rubber compoundsfor the productionof efficientpower details ofdepreciation |
||||||||
|
||||||||
Soft |
||||||||
VI-2м |
ИРП-1346 |
СКИ-3+СКД |
40-50 |
-60 tо +100 |
In the environment of air and in contact with water, weak acids and alkalies |
|||
VI-2м |
ИРП-1347 |
СКИ-3+СКД |
45-60 |
-50 tо +80 |
||||
VI-2м |
6621 |
СКИ-3+СКД |
35-50 |
-50 tо +80 |
||||
VI-2м |
2959 |
НК |
45-60 |
-50 tо +80 |
||||
VI-2м |
7-1847 |
НК |
35-50 |
-50 tо +80 |
||||
|
|
|
|
|
|
|||
Half-hard |
||||||||
VI-2с |
7-ИРП-1315 |
СКИ-3 |
50-70 |
-30 tо +70 |
In the environment of air and in contact with water, weak acids and alkalies |
|||
VI-2с |
120 |
НК |
65-75 |
-45 tо +80 |
||||
VI-2с |
7-6620 |
СКИ-3 |
50-60 |
-50 tо +80 |
||||
VI-2с |
1127 |
СКИ-3+СКМС-30АРКМ-15 |
50-65 |
-30 tо +70 |
||||
|
|
|
|
|
|
|||
|
|
|
|
|
|
|||
|
|
|
|
|
|
|||
Increased hardness |
||||||||
VI-2п |
ИРП-1348 |
СКИ-3+СКД |
65-80 |
-50 tо +80 |
In contact with oils and fuels |
|||
VI-2п |
2462 |
НК |
60-80 |
-40 tо +80 |
||||
|
|
|
|
|
||||
|
||||||||
Soft |
||||||||
VI-2м |
ИРП-1352 |
СКН-18 |
35-65 |
-50 tо +100 |
In contact with oils and fuels |
|||
|
|
|
|
|
||||
Half-hard |
||||||||
VI-2с |
8470 |
БНКС-18+ БНКС-28 |
50-65 |
-30 tо +100 |
In contact with oils and fuels |
|||
|
|
|
|
|
||||
Increased hardness |
||||||||
VI-2п |
4326 |
СКН-18 |
65-80 |
-45 tо +100 |
In contact with oils and fuels |
|||
|
|
|
|
|
||||
VII. The rubber compoundsincreased wear resistance |
||||||||
1. For air |
||||||||
Soft |
||||||||
VII-1м |
44-3 |
СКИ-3+СКД |
35-65 |
-40 tо +70 |
For air |
|||
|
|
|
|
|
|
|||
Half-hard |
||||||||
VII-1с |
6252ф |
СКИ-3+СКД |
50-70 |
-40 tо +70 |
For air |
|||
VII-1с |
51-1625 |
СКИ-3 |
50-70 |
-40 tо +70 |
||||
|
|
|
|
|
|
|||
Increased hardness |
||||||||
VII-1п |
51-1632 |
СКЭПТ-30,40,50 |
70-85 |
-30 tо +100 |
For air |
|||
VII-1п |
ИРП-1231 |
СКИ-3+СКМС-30АРКМ-15 |
60-80 |
-55 tо +70 |
||||
VII-1п |
ИРП -1232 |
СКИ-3+ chloroprene, СКД |
60-80 |
-55 tо +70 |
||||
|
|
|
|
|
|
|||
2. Petrol and oil resistant |
||||||||
Increased hardness |
||||||||
VII-2п |
ИРП-1226 |
БНКС |
70-80 |
-20 tо +100 |
In contact with oils and fuels |
|||
VII-2п |
ИРП-1293 |
СКН-40с |
65-80 |
-10 tо +100 |
||||
VII-2п |
ИРП-1294 |
СКН-40с |
65-80 |
-20 tо +100 |
||||
|
|
|
|
|
||||
IX.Rubber compoundsfor the production of harf-ebony andebonyproducts andliningsfor shafts |
||||||||
Soft |
||||||||
IX-м |
2566 |
СКМС-30АРКМ-15+СКИ-3 |
40-60 |
-30 tо +70 |
|
|||
Half-hard |
||||||||
IX-с |
1976 |
СКМС-30АРКМ-15 |
50-70 |
-30 tо +70 |
|
|||
IX-с |
51-1627-1 |
СКМС-30АРКМ-15+СКИ-3 |
50-70 |
-30 tо +70 |
|
|||
Increased hardness |
||||||||
IX-Э |
51-1627 |
СКМС-50+СКИ-3 |
85-100 |
2 tо +70 |
|
|||
|
|
|
|
|
|
|||
XII. Rubbermixturefor thesplicing and repairof conveyor belts. |
||||||||
XII-1.2-3 |
1602 (аналог 2-990УС) |
СКМС-30АРКМ-15+СКИ-3+хлоропреновый |
55-75 |
-25 tо +70 |
For the lining fabric belts in a flameproof version |
|||
XII-2.1-1 |
2-832 ЭР (аналог 26425УС) |
СКИ-3 |
- |
-45 tо +60 |
For applying interlayer on fabric of rubber fabric belts |
|||
|
|
|
|
|
|
|||
XII-2.2-1 |
2-757 |
СКИ-3+СКД+ СКМС-30АРКМ-15 |
- |
-45 tо +60 |
For the lining of rubber-bands in a fire-resistant performance |
|||
XII-2.1-1 |
2-832 |
СКИ-3 |
- |
45 tо +60 |
For applying interlayer on fabric of rubber fabric belts |
|||
ХIV. Rubbermixtureusedin the shoeindustry. |
||||||||
ХIV |
101-ЭР (181-РК-1) |
СКМС-30АРКМ-15 |
60-75 |
- |
- |
|||
ХIV |
101-1-ЭР (181-2) |
СКМС-30АРКПН |
60-75 |
- |
- |
|||
ХIV |
103 –ЭР (553) |
СКМС-30АРКПН |
50-70 |
- |
- |
|||
ХIV |
103–1-ЭР (553-РК-1) |
СКМС-30АРКМ-15 |
48-68 |
- |
- |